How hot is too hot to pour concrete?

ACI 301 and 305.1 cap concrete at 95 °F when it is discharged. Heat alone isn’t the test: 95 °F air, 90 °F concrete, 30% humidity and a 10 mph wind evaporate about 0.24 lb/ft²/h, past the 0.2 where plastic shrinkage cracks are expected.

A hot day on its own won’t stop a pour. What goes wrong in the heat is that concrete sets faster, needs more water and dries at the surface before it has set. Here is the temperature limit the American Concrete Institute (ACI) gives, why wind and humidity matter as much as the thermometer, and what the National Ready Mixed Concrete Association (NRMCA) and the bag say to do about it.

Figures checked by Matt Tay (Tay Tzu Haw)

What counts as hot weather?

ACI’s Guide to Hot Weather Concreting (ACI 305R-20) doesn’t give a single temperature. It defines hot weather as any combination of high air temperature, high concrete temperature, low relative humidity, high wind speed and sun that harms fresh or hardened concrete by speeding up moisture loss and the cement’s reaction.

That is why the same 90 °F can be fine one day and a problem the next. ACI says the precautions needed on a windy, sunny day are stricter than on a calm, humid one, even at the same air temperature, and that drying conditions can occur at lower temperatures too. NRMCA’s CIP 12 sheet adds that high humidity tends to reduce the effects of heat.

The 95 °F limit

The number most specifications use is for the concrete, not the air. ACI explains that ACI 301-20 and ACI 305.1-14 limit the concrete temperature to 95 °F (35 °C) at the time of discharge from the truck, for ordinary work such as pavements and buildings. A mix that will run hotter has to be backed by past field experience or testing before the pour, and submitted to the engineer.

You may still see 90 °F in older specs. ACI 305R itself warns that hot weather is too complex to manage by a maximum concrete temperature alone, and NRMCA notes the purchaser can waive the limit if the concrete is workable enough without extra water. So treat 95 °F as the line to talk to the supplier about, not as a guarantee that anything cooler is safe.

What happens as concrete gets hotterFigureSource
Maximum concrete temperature at discharge95 °F (35 °C)ACI 301-20, ACI 305.1-14
28-day strength of test cylinders cured at 100 °F (38 °C) for the first day10 to 15% lowerACI 305R-20
Chilled mixing water can cool the concrete byUp to 10 °F (6 °C)NRMCA CIP 12
Ice in place of some mixing water can cool it byUp to 20 °F (12 °C)NRMCA CIP 12
Don’t add water to concrete older than1½ hoursNRMCA CIP 12

The 100 °F figure is ACI’s, for test cylinders. NRMCA says the same of the slab: concrete cured hot at an early age won’t be as strong later as the same concrete cured at around 70 °F, and hot concrete needs more water, which lowers strength and durability if it is added on site.

Why wind and humidity matter as much as heat

Plastic shrinkage cracks form when the surface loses water faster than bleed water can rise to replace it. NRMCA’s CIP 5 lists the conditions that drive that: wind over 5 mph, low humidity, and high air or concrete temperatures. The evaporation rate calculator puts them into one number with Uno’s equation for the ACI 305 nomograph:

E = 5 × ([Tc + 18]^2.5 − r × [Ta + 18]^2.5) × (V + 4) × 10⁻⁶Tc concrete °C, Ta air °C, r humidity (fraction),V wind km/h, E in kg/m²/h

Kestrel’s risk bands, from ACI 305: under 0.1 lb/ft²/h cracks aren’t expected; between 0.1 and 0.2 they may occur and precautions are recommended; over 0.2 they are expected unless the surface is protected.

Worked example: a July driveway

  • Afternoon: air 95 °F, concrete 90 °F, 30% humidity, a 10 mph wind. The equation gives about 0.24 lb/ft²/h, over 0.2 (run these numbers).
  • Same afternoon, concrete cooled 10 °F with chilled water, as CIP 12 says is possible: 80 °F concrete gives about 0.15 lb/ft²/h, still in the precautions band.
  • Same afternoon, wind cut to 3 mph by a windbreak: about 0.11 lb/ft²/h, just over 0.1. Calm air brings it to about 0.05.
  • Early morning instead: air 80 °F, concrete 85 °F, 60% humidity, 5 mph. About 0.09 lb/ft²/h, under 0.1 (run these numbers).

Wind does more than any other single change here, which is why NRMCA puts windbreaks first. Moving the pour to the morning helps on every count at once: cooler concrete, cooler air, more humidity and usually less wind.

Planning a hot-day pour

  1. Pick the time. NRMCA says to avoid the hottest part of the day. For plastic shrinkage it suggests starting late in the afternoon or evening, or early in the morning in very hot weather, when the concrete’s temperature is easier to control.
  2. Talk to the supplier. The ready-mix producer can use retarding or water-reducing admixtures, chilled water or ice, and shaded or sprinkled aggregate to keep the mix workable and cooler. Schedule deliveries so trucks can discharge as soon as they arrive.
  3. Have enough hands. Concrete sets faster in the heat and finishing has to keep up, so plan the crew and the rate of delivery together.
  4. Dampen, don’t flood. On dry or hot days, dampen the subgrade, forms and reinforcement before placing, without leaving standing water (NRMCA). Quikrete’s instructions also start by dampening the subgrade.
  5. Block the wind and sun. Windbreaks, sunshades and a fog spray upwind of the slab all lower evaporation (CIP 5). An evaporation retardant sprayed after screeding is another option.

Don’t sprinkle water on the surface

Water added to make a drying slab easier to finish weakens the surface. NRMCA says not to do it, and not to add more water at the site than the mix was designed for. Begin final finishing when the water sheen has left the surface.

Curing in the heat

Start curing as soon as finishing is done. NRMCA’s hot-weather rule is to keep curing for at least 3 days, with wet burlap under plastic sheeting, a liquid membrane curing compound, or water. A white-pigmented curing compound reflects heat and shows where it has been applied. Quikrete’s data sheet for its Concrete Mix says to cure for 5 days when it’s 70 °F or warmer; hot, dry or windy weather takes water from the concrete that it needs to gain strength, and leads to shrinkage cracking.

Watch for a cool night after a hot day. NRMCA warns that a slab placed in the heat and followed by a sharp drop in temperature can crack from the change, so keep covers on overnight. For how long to stay off the slab, see concrete curing time; for the opposite season, see how cold is too cold to pour.

Questions people ask

Can you pour concrete at 100 degrees?
It can be done, but the concrete itself should be no hotter than 95 °F when it leaves the truck (ACI 301-20 and 305.1-14), and at that air temperature the surface can dry fast. Pour early in the morning, ask the supplier about chilled water or a retarder, block the wind, and start curing as soon as you finish.
What is the maximum temperature for pouring concrete?
ACI 301-20 and ACI 305.1-14 limit the concrete temperature to 95 °F (35 °C) at discharge for ordinary work. Air temperature has no single limit: ACI 305R judges hot weather by air and concrete temperature, humidity, wind and sun together.
Is it better to pour concrete in the morning or the evening in summer?
Either beats the afternoon. NRMCA suggests late afternoon or evening to limit plastic shrinkage cracking, and early morning in very hot weather, when the concrete’s temperature is easier to control. Check the evaporation rate for the hours you are considering.
How long should concrete be kept wet in hot weather?
NRMCA says to cure for at least 3 days in hot weather, with wet burlap and plastic, a curing compound or water. Quikrete’s data sheet says 5 days for its Concrete Mix at 70 °F or warmer.

Sources for the numbers on this page

  1. American Concrete Institute: ACI 305R-20 Guide to Hot Weather Concreting — preview (definition of hot weather, early curing temperature) · checked
  2. American Concrete Institute: FAQ: placing concrete in a hot climate (95 °F maximum at discharge, ACI 301-20 and 305.1-14) · checked
  3. National Ready Mixed Concrete Association: CIP 12 — Hot weather concreting (cooling the mix, jobsite water, curing) · checked
  4. National Ready Mixed Concrete Association: CIP 5 — Plastic shrinkage cracking (precautions) · checked
  5. Kestrel Instruments: How to prevent plastic shrinkage cracks (Uno evaporation equations and risk bands) · checked
  6. Quikrete: Concrete Mix No. 1101 — technical data sheet (bag yields, strength gain, curing) · checked

Corrections and updates are logged on the sources page.