How cold is too cold to pour concrete?

ACI counts it as cold weather once the air falls, or is forecast to fall, below 40 °F during the protection period. Fresh concrete freezes below about 25 °F; keep it from freezing until it reaches 500 psi, about two days, and place a slab under 12 in thick at 55 °F or warmer.

There is no single air temperature below which concrete can’t be poured. What matters is whether you can place it warm enough and keep it from freezing until it is strong enough to survive. Here are the thresholds the American Concrete Institute (ACI) and the National Ready Mixed Concrete Association (NRMCA) give, what the bag says, and how to decide whether to pour or wait.

Figures checked by Matt Tay (Tay Tzu Haw)

When does cold weather start?

ACI’s Guide to Cold Weather Concreting (ACI 306R-16) says cold-weather conditions exist when the air temperature has fallen to, or is expected to fall below, 40 °F (4 °C) during the protection period: the time the concrete needs to be kept from harm by the cold. So the forecast for the next two or three nights matters as much as the temperature while you pour.

You will still see an older test, which NRMCA’s CIP 27 sheet gives: more than 3 days in a row with an average daily temperature under 40 °F, and the air no warmer than 50 °F for more than half of any 24 hours. The 2016 guide replaced it with the simpler 40 °F rule above. Either way, 40 °F is the line where special precautions start, not the line where pouring stops.

The temperatures that matter

ThresholdFigureSource
Cold-weather precautions startAir at or below 40 °F (4 °C)ACI 306R-16
Fresh concrete freezesBelow about 25 °F (−4 °C)NRMCA CIP 27
Strong enough to survive one freeze500 psi (3.5 MPa), about 2 daysACI 306R-16, NRMCA CIP 27
Strong enough for repeated freezing and thawing3,500 psi (24 MPa)NRMCA CIP 27
Setting time doublesFor every 20 °F (10 °C) the concrete is colderNRMCA CIP 27

Concrete that freezes while it is still fresh can lose more than half its potential strength, NRMCA says, and it won’t be durable. That is why the 500 psi mark matters: ACI explains that by then the concrete is no longer saturated enough for freezing to do that damage. At 50 °F most well-proportioned mixes reach it within 48 hours.

How warm the concrete should be when placed

The number to watch is the temperature of the concrete itself, not the air. NRMCA’s recommended minimums as placed depend on how thin the section is, because thin pieces lose their heat fastest:

Smallest dimension of the sectionConcrete temperature as placed, at least
Less than 12 in (300 mm): slabs, walks, driveways55 °F (13 °C)
12–36 in (300–900 mm): footings, thick walls50 °F (10 °C)
36–72 in (900–1,800 mm)45 °F (7 °C)

Both ACI and NRMCA say not to go more than 20 °F above these: hotter concrete needs more mixing water, loses slump faster and cracks more easily. For a 4 in patio that means concrete between 55 and 75 °F. NRMCA notes that the ready-mix producer can control the concrete’s temperature to meet it, so ask when you order. Bagged mix starts at the temperature of the bags and the water, so keep both somewhere warm.

What the bag says

For its standard Concrete Mix, Quikrete’s data sheet says:

  • Protect the concrete from freezing during the first 48 hours.
  • Use plastic sheeting and insulation blankets if temperatures are expected to fall below 32 °F (0 °C).
  • Don’t apply a curing compound if rain, or temperatures below 50 °F (10 °C), are expected within 24 hours.
  • Cure for 7 days when it’s between 50 and 70 °F, against 5 days at 70 °F or warmer.

That 48 hours lines up with ACI’s two days to 500 psi. The extra curing time below 70 °F is the slower strength gain at work: the colder the concrete, the longer everything takes.

So how cold is too cold?

Put the sources together and the question becomes three checks:

  1. Is the ground thawed? NRMCA says to clear snow and ice and to have every surface the concrete touches, including the subgrade, above freezing. Never pour on frozen ground.
  2. Can the concrete go in at 55 °F or warmer? For a slab under 12 in thick, that is the minimum. In practice this means ready-mix ordered warm, or bags and water stored indoors.
  3. Can you keep it above freezing for two days? If the forecast drops below 32 °F in the 48 hours after the pour, you need blankets or insulation over it before the sun goes down. If you can’t supply them, wait for a warmer spell.

If all three are yes, a cold day is workable, and NRMCA notes a cooler start often ends with higher ultimate strength. If any is no, the risk is concrete that freezes fresh: weaker, and not durable.

Accelerators don’t stop freezing

An accelerating admixture makes concrete set and gain strength faster, but NRMCA is clear that it doesn’t keep it from freezing and doesn’t replace protection. Calcium chloride, the common one, shouldn’t exceed 2% of the cement’s weight, and isn’t for concrete with steel reinforcement where corrosion is a concern.

Cold, dry wind still dries fresh concrete

Plastic shrinkage cracks are usually a summer problem, but evaporation depends on how much warmer the concrete is than the air, not on the heat of the day. Warm concrete placed into cold, dry, windy air can lose surface water faster than on a mild day. The evaporation rate calculator uses Uno’s equation for the ACI 305 nomograph:

E = 5 × ([Tc + 18]^2.5 − r × [Ta + 18]^2.5) × (V + 4) × 10⁻⁶Tc concrete °C, Ta air °C, r humidity (fraction),V wind km/h, E in kg/m²/h

Worked example: a winter patio pour

  • Concrete placed at 60 °F, inside NRMCA’s 55–75 °F band for a slab.
  • Air at 30 °F, 40% humidity, a 15 mph wind.
  • The equation gives about 0.17 lb/ft²/h, past the 0.1 lb/ft²/h where precautions are recommended (run these numbers).
  • Out of the wind, at 0 mph, the same pour loses about 0.03 lb/ft²/h, well under it.

For comparison, 70 °F concrete on a 70 °F day at 50% humidity and a 10 mph wind comes to just under 0.1. A windbreak and covering the slab as soon as it is finished deal with both the cold and the drying. NRMCA adds that the surface shouldn’t dry before it sets, and that water curing isn’t recommended when freezing is near: use plastic sheets or curing paper instead.

Protecting it after the pour

  • Cover the slab with insulated blankets, or straw under plastic sheeting, as NRMCA lists. Edges and corners lose heat first, so lap the covers well past them.
  • Vent fuel-burning heaters in any enclosure. NRMCA warns that their exhaust can carbonate the fresh surface, which leaves it dusting.
  • Leave forms on for 1 to 7 days depending on how fast the concrete is gaining strength, the weather and what will load it.
  • Take the covers off gradually. A difference of more than about 35 °F (20 °C) between the surface and the inside can crack it, and ACI says to let the surface cool over the following 24 hours.
  • Use air-entrained concrete for anything outdoors that will see freezing and thawing while wet, such as driveways and walks.

Questions people ask

Can you pour concrete at 30 degrees?
Yes, if the ground isn’t frozen, the concrete goes in warm enough (55 °F for a slab under 12 in thick, per NRMCA) and you can keep it from freezing for about two days with blankets or an enclosure. Without that protection, wait: concrete that freezes fresh can lose more than half its strength.
What is the lowest temperature to pour concrete without precautions?
ACI’s 2016 guide treats any time the air is at or below 40 °F, or is forecast to fall below it during the protection period, as cold weather that calls for precautions. Above that, with no frost in the forecast for the next two days, normal practice applies.
How long does concrete need to be protected from freezing?
Until it reaches 500 psi, which ACI says most mixes reach within 48 hours at 50 °F, and Quikrete’s data sheet says 48 hours for its Concrete Mix. Concrete that will be wet and freeze repeatedly should be protected from freezing and thawing cycles until about 3,500 psi, NRMCA says.
Can you pour concrete on frozen ground?
No. NRMCA says to remove snow and ice and have the subgrade and anything else the concrete touches above freezing before placing it. Thawing the ground may mean insulating or heating it before the pour.

Sources for the numbers on this page

  1. American Concrete Institute: ACI 306R-16 Guide to Cold Weather Concreting — preview (definition of cold weather, 500 psi protection) · checked
  2. National Ready Mixed Concrete Association: CIP 27 — Cold weather concreting (placement temperatures, freezing, protection) · checked
  3. Quikrete: Concrete Mix No. 1101 — technical data sheet (bag yields, strength gain, curing) · checked
  4. Kestrel Instruments: How to prevent plastic shrinkage cracks (Uno evaporation equations and risk bands) · checked